Typical Composition of all-weld Metal
Mechanical Test of weld Metal
Tempered, 700 oC /2h/furnace up to 300 oC/air
– Deposition efficiency 115 %
Operating Data
Welding Positions
- All, except vertical down
Polarity
- DC (+)
Industrial Zone A1, 10th of Ramadan City, Egypt

99 El Sebak Street
Maryland - Heliopolis - Cairo - Egypt
+2012 2100 5111
+2010 0885 1811
Description It is suitable for cryogenic applications where it’s crack-free, it is ideal for quenching and tempering, where it has good resistance to caustic cracking, excellent creep resistance in moderate time, has good application for severe steam boiler conditions and superheated heat exchanger. |
| C | Si | Mn | Mo | P | S | Cr | |
| Wt. % | 0.06 | 0.25 | 0.80 | 0.5 | 0.02 | 0.02 | 1.2 |
| Typical According to ASME II part C/SFA 5.5 | 0.05 – 0.12 | 0.80 max. | 0.90 max. | 0.4-0.65 | 0.03 max. | 0.03 max. | 1.0-1.5 |
| Heat Treatment | Yield Strength 0.2% | Tensile Strength | Elongation L0=5d0 | Impact values In J CVN | ||
| MPa | MPa | % | +20 oC | -20 oC | -50 oC | |
| Tempered at 690 oC / 1h | 480 | 570 | 24 | 120 | 80 | 60 |
| Average Reference According to ASME II part C/SFA 5.5 | ≥ 460 | ≥ 550 | ≥ 19 | N.S |
Tempered, 700 oC /2h/furnace up to 300 oC/air
– Deposition efficiency 115 %
| 2.5mm | 3.25 mm | 4.0mm | 5.0mm | |
| L mm | 350 | 350 | 350/450 | 350/450 |
| Amps A | 80-110 | 110 – 145 | 130-190 | 160-230 |