Typical Composition of all-weld Metal
Mechanical Test of weld Metal
Operating Data
| Re – drying: if necessary: 300 – 350 ºC, min. 2 h . |
Deposition efficiency = 110 %
Welding Positions
- All, except vertical down
Polarity
- DC (+)
Industrial Zone A1, 10th of Ramadan City, Egypt

99 El Sebak Street
Maryland - Heliopolis - Cairo - Egypt
+2012 2100 5111
+2010 0885 1811
Basic coated engineered electrode for high-quality welds. Excellent strength and toughness properties down to – 50ºC, Metal recovery approx.; 110 %. Good weldability in all position except for vertical-down, Very low Hydrogen content. Suitable for welding steels with low purity and high carbon content. Welding in steel construction, boilers and tanks manufacture, vehicle construction, shipbuilding, and machine construction as well as for buffer layers on build ups on high carbon steels. Especially suitable for off-shore construction. |
| C | Si | Mn | P | S | Ni | Cr | Mo | v | |
| Wt. % | 0.07 | 0.42 | 0.75 | 0.012 | 0.011 | 0.02 | 0.02 | 0.02 | 0.02 |
| Typical According to ASME II part C/SFA 5.1 | 0.15 max. |
0.75 max. |
1.60 max. |
0.035 max. |
0.035 max. |
0.30 max. |
0.20 max. |
0.30 max. |
0.08 max. |
| Heat Treatment | Yield Strength | Tensile Strength | Elongation L0=5d0 | Impact values In J CVN |
| N/mm2 | N/mm2 | % | -50 oC | |
| Untreated | 440 | 545 | 32 | 110 |
| Typical According to ASME II part C/SFA 5.1 | ≥ 400 | ≥ 490 | ≥ 22 | ≥ 27 |
| Re – drying: if necessary: 300 – 350 ºC, min. 2 h . |
| 2.5mm | 3.25 mm | 4.0mm | 5.0mm | |
| L mm | 350 | 350/450 | 350/450 | 350/450 |
| Amps A | 80 -110 | 100 -140 | 130 -180 | 180-230 |
Deposition efficiency = 110 %